Why PVC Turns Yellow During Extrusion: Resin or Stabilizer

Either one can turn PVC yellow in the extruder, and so can the line itself. The resin sets the number of weak points along the chain where hydrogen chloride starts to come off, and the stabilizer sets how long the compound holds out against that loss. Process conditions, chiefly a melt running hotter than the barrel settings show, can yellow a sound compound too.

Yellowing that appears months after installation on the face exposed to sunlight is UV degradation, a separate problem. This article covers colour the extrudate already has when it leaves the die.

When the Resin Is the Cause

The resin is the cause when it brings more of the weak points where dehydrochlorination starts, or more leftover polymerization initiator, than a resin that runs clean with the same stabilizer. These structural defects are built into the polymer during polymerization, and their amount depends on how the resin was made, so two resins run with the same stabilizer start from different heat stability.

Weak Points Built Into the Resin

The weak points are chlorine atoms in unstable positions: internal allylic chlorides next to a double bond, and tertiary chlorides at branch points. Every commercial PVC contains them.

Polymerization initiator left in the resin adds a separate effect: it starts dehydrochlorination early, which shows as early discolouration.

Lot-to-Lot Variation

Heat stability does vary between resin lots and between producers, because the weak-point content moves with polymerization temperature and conversion. No published data puts a number on how much.

The resin certificate will usually not show it. Under China’s general-purpose suspension PVC standard, GB/T 5761-2018, heat whiteness is a type-inspection item rather than a batch test, required at least once every three months and again when the producer changes its process, raw materials or equipment.

A heat-whiteness figure printed on a datasheet is therefore a limit the grade meets, and may not be a measurement of the lot you received. A processor chasing lot-to-lot yellowing has to test incoming lots itself.

Moisture in the Resin

Water in the resin speeds up dehydrochlorination, but no published work ties a resin moisture level to yellowing at extrusion temperatures, so moisture is a secondary suspect. Moisture in a rigid compound shows first as bubbles in the extrudate.

Unlike heat stability, moisture is on the certificate. Volatile matter is a batch-release item under GB/T 5761-2018. The volatile-matter limits on Bastone’s SG-series and S-1300 suspension grades sit between 0.20 % and 0.40 %, depending on grade, so a wet lot normally shows on its certificate.

When the Stabilizer Is the Cause

The stabilizer is the cause when its protection runs out before the melt leaves the die, or when it holds colour early and fails later in the run.

Too Little Stabilizer for the Temperature and Residence Time

The dosage is too low when the compound’s stability time at your actual melt temperature is shorter than the time the slowest-moving melt spends in the barrel and die.

The sign is yellowing that follows melt temperature and time: it worsens when the line runs faster or hotter, and builds up the longer the die has been running. Confirm it by measuring the stability time of a fused sample of the compound against a control that ran clean.

Wrong Stabilizer Type for the Run

A compound that is yellow from the start lacks initial-colour protection; one that leaves the die white and then turns yellow or brown suddenly, late in the run, lacks long-term stability. Zinc-rich calcium-zinc systems are the classic case of the second.

Zinc soap replaces labile chlorine and gives excellent early colour, but the zinc chloride it forms catalyses rapid dehydrochlorination, known as zinc burning, and calcium soap delays it.

A stabilizer built for long-term stability can also hold through a long run yet give the extrudate a yellowish start.

Stabilizer Degraded Before It Reached the Extruder

Part of the stabilizer’s capacity is spent before extrusion when the dry blend runs too hot in the high-speed mixer, or when the stabilizer has been stored open to humid air or past its shelf life. The result looks like too little stabilizer although the batch sheet shows the right dosage. A blend made with stabilizer from a fresh, sealed container separates the two.

Poor Dispersion in the Dry Blend

Uneven dispersion shows as local yellow or brown streaks and specks in extrudate that is otherwise a good colour. It points to the mixing step rather than to the stabilizer’s type or dosage.

When Neither Is the Cause

A sound resin and stabilizer still yellow when the process gives the melt more heat or more time than the formulation was built for. The most common case is a melt running hotter than the barrel settings suggest.

A zone sitting above its set point with cooling on (zone override) is the sign. Lowering the set points often barely moves the melt temperature.

Measure the melt directly with a hand-held pyrometer or an immersion probe; the pressure/temperature transducer in the die is not a reliable melt reading. For a large change in melt temperature, the fix is usually in the screw design.

Three other process conditions yellow a sound compound:

  • Dead spots in the melt path: material that stagnates in a flat-plate die or an unstreamlined adaptor stays hot long enough to degrade, then breaks loose as discoloured streaks.
  • Reactive metal: carbon steel, aluminium, brass or copper in the melt path reacts with PVC. A new barrel can also discolour the melt at the metal surface for its first few days of running.
  • Regrind: reground extrudate has already been through one heat history, so a high regrind share shortens the stability time left in the blend.

How to Tell Resin From Stabilizer

Rule out the process first, read the yellowing pattern for a first suspect, then confirm with a trial that changes one ingredient at a time against a control. If the yellowing started when the line changed (a new die, a higher rate, a screw change) and the ingredients did not, look at the process before either ingredient.

Read the Yellowing Pattern

The pattern narrows the suspects, but it does not prove which ingredient is at fault:

  • Yellow from the first metre, evenly: initial-colour protection is short. A resin with more weak points or leftover initiator and a stabilizer weak on early colour both look like this.
  • White at first, then sudden yellow or brown late in the run: long-term capacity is running out, as in zinc burning or a dosage too low for the residence time.
  • Worse at higher rate or melt temperature: the stabilizer’s stability time is shorter than the melt’s time at that temperature.
  • Streaks or specks in good-coloured extrudate: poor dispersion in the dry blend, or a dead spot in the die.
  • Started with a new resin lot or resin source: the resin is the first suspect.
  • Started with a new stabilizer drum or a mixer change: the stabilizer is the first suspect.

Swap One Variable at a Time

Change one ingredient per trial and hold everything else: other ingredients, mixer cycle, temperature profile and line rate. Keep a retained sample of every resin lot that runs clean, so you have a reference to swap in.

  • Resin trial: run the suspect resin and the reference resin, each with stabilizer from a fresh, sealed container. If only the suspect resin yellows, the resin is the cause.
  • Stabilizer trial: run the reference resin with the current stabilizer and with fresh stabilizer. If only the current stabilizer yellows, the stabilizer is the cause.

To compare in the lab rather than on the line, test each compound’s stability time against the clean control: an ISO 182 stability-time method, or the thermal-stability and colour-hold procedures of ASTM D2538 on a torque rheometer. The ISO 182 methods are not written for dry blends, so fuse or compound each trial blend before testing.

Test the Incoming Resin’s Heat Stability

The test built for resin powder is the heat-whiteness method of GB/T 15595: a resin sample is heated, at 160 °C for 10 minutes under GB/T 5761, and its whiteness measured. The result is a relative comparison, so test each incoming lot beside a retained sample of a lot that ran clean.

The ISO 182 methods are compound tests: Congo red (ISO 182-1) is recommended for compounds only, and Part 2 (pH) and Part 3 (conductometric) accept resin powder only under conditions agreed between the parties.

Newsletter Updates