DOP is one of the most effective plasticizers in terms of plasticizing performance, while also being cost-effective. Therefore, DOP (Dioctyl Phthalate) is a most used plasticizer“. BASTONE is the leading DOP manufacturer and supplier in China, with years of experience as a reliable producer and exporter of plasticizers.

DOP Production Process

DOP Producer continuous prodution process

Phthalic anhydride reacts with 2-ethylhexanol in a molar ratio of 1:1.6 at 120°C for monoesterification. The reaction proceeds continuously into a diesterification reactor.

At 130–150°C and 7.9 kPa, with sulfuric acid catalyst (0.5% of total feed), the reaction continues to form the diester (DOP).

The crude ester product is first washed with water at 50°C using 1/5 of the total volume, followed by neutralization with 2%–3% sulfuric acid at 60–70°C. Then, it is further neutralized at a 1:1 ratio with water at 70–80°C, followed by a final hot water wash.

Then, 0.1% activated carbon is added and the mixture is deacidified and decolored at 150°C and 3.9 kPa under vacuum. Finally, the product is filtered to obtain purified DOP.

How DOP is made brief production process BASTONE

Specification

AppearanceTransparent oily liquid
Chroma≤30
Purity≥99.5%
Density(20℃)0.982-0.988 g/cm3
Flash Point≥196℃
Acidity≤0.030%
Water≤0.10%
BASTONE is the leading DOP Producer (manufacturer) in China
China DOP Producer;Plasticizer DOP

BASTONE Plasticizers Enhance the performance of your PVC products. Find costing-saving plasticizer DINP, DOTP, DOP, DOP, DPHP, DBP, DIBP at our site https://bastoneplasti.wpenginepowered.com

Newsletter Updates

Enter your email address below and subscribe to our newsletter