This article highlights actionable insights for manufacturers seeking to refine PVC foam formulations while emphasizing
1. Reference Formula/ Plasticizer DOP dosage
Material | PHR[Parts by weight per hundred parts of resin] |
---|---|
PVC | 100 |
Organotin stabilizer | 2 |
PE wax | 1 |
Ester lubricant | 3 |
Stearic acid | 0.3 |
CaCO₃ | 10 |
ACR | 6 |
Plasticizer DOP | 2 |
2. Key Insights with Plasticizer DOP
2.1. DOP Enhances Melt Flow and Processability
Rheological Benefits : Adding DOP reduced both melting torque and equilibrium torque by up to 30% (at 2 phr), improving PVC’s flow characteristics and lowering extrusion pressure. Optimal Dosage : 2 phr DOP achieved the best balance between melt elasticity (for cell nucleation) and melt strength (to prevent collapse).
2.2 Microstructure Optimization
SEM Analysis : 2 phr DOP : Uniform, fine cells (optimal morphology).
Density Control : 2 phr DOP yielded the lowest density (~0.5 g/cm³) due to uniform cell growth.
2.3 Mechanical Performance Trends
Tensile Strength : Decreased by 1.9% (0–2 phr) and 16.9% (2–4 phr) as DOP weakened intermolecular bonds. Elongation at Break : Peaked at 2 phr (improved flexibility) but dropped with higher DOP (structural instability). Flexural & Impact Strength : Declined consistently with DOP content due to reduced melt strength.
2.4. Practical Guidelines
Recommended DOP Level : 2 phr balances processability, cell uniformity, and mechanical integrity. Avoid Overuse : Excess DOP (>2 phr) risks foam collapse and inferior performance.